MENU Buscar NSK - Motion & Control
Damage Condition Possible Causes Countermeasures
Dull or cloudy spots appear on surface along with light Wear. From such dull spots, tiny Cracks are generated downward to a depth of 5-10 µm. Small particles fall off and minor Flaking occurs widely.
  • Unsuitable lubricant
  • Entry of debris into lubrication
  • Rough surface due to poor lubrication
  • Surface roughness of mating rolling parts
  • Select a proper lubricant
  • Improve the sealing mechanism
  • Improve the surface finish of the rolling mating parts

 

Click a photo to enlarge it

Peeling 1

Part: Inner ring of a spherical roller bearing
Symptom: Rounded areas of Peeling
Cause: Poor lubrication

Peeling 2

Part: Enlargement of damage “Peeling 1”

Peeling 3

Part: Convex rollers of damage “Peeling 1”
Symptom: Rounded areas of Peeling on the center of the rolling surfaces
Cause: Poor lubrication

Peeling 4

Part: Outer ring of a spherical roller bearing
Symptom: Peeling occurs near the shoulder of the raceway over the entire circumference
Cause: Poor lubrication

Cookies no site da NSK

Nós usamos cookies para garantir que nós damos-lhe a melhor experiência em nossos sites e aplicações web. Ao continuar sem alterar as configurações do navegador, vamos supor que você deu o seu consentimento para receber cookies. No entanto, você pode alterar a configuração de cookies do navegador a qualquer momento.